Results 1 to 7 of 7
  1. #1
    smatros's Avatar
    smatros is offline Senior Member
    Join Date
    Dec 2008
    Location
    Slovenia, EU
    Posts
    184

    Default Uv coating problem on xerox prints

    We are trying to uv coat digital prints with glossy coating for digital (drytac) on a simple no-name uv coater. The problem we get is "wrinkled" gloss, like some kind of wavy surface. The problem is not present on some test coatings done on offset prints with another coating, so i guess it is not the machine. Any advice on how to get clean smooth glossy surface? Thank you in advance.
    Smatros print & natisni.si - small format, large format, flatbed, dtg, laser engraving & more in EU

  2. #2
    NeedtoKnow's Avatar
    NeedtoKnow is offline Junior Member
    Join Date
    Dec 2009
    Posts
    1

    Default UV coating problem

    You may be experiencing a chemical reaction between the paper coating and the UV. I suggest you coat a blank sheet of stock to see if you get the same results.

  3. #3
    oxburger's Avatar
    oxburger is offline Senior Member
    Join Date
    Oct 2007
    Posts
    510

    Default

    There is probably a difference where the UV is hitting paper vs. the UV hitting toner on the paper. It's probably soaking in in areas and not in others causing the "wave" problem.
    By the time I walk out of here, I'm going to be a lean, mean, prepress machine...

  4. #4
    Dieter Zang is offline Junior Member
    Join Date
    Nov 2009
    Location
    Germany, Reulingen
    Posts
    2

    Default

    Quote Originally Posted by smatros View Post
    We are trying to uv coat digital prints with glossy coating for digital (drytac) on a simple no-name uv coater. The problem we get is "wrinkled" gloss, like some kind of wavy surface. The problem is not present on some test coatings done on offset prints with another coating, so i guess it is not the machine. Any advice on how to get clean smooth glossy surface? Thank you in advance.
    Problem is that the Xerox print does have a special surface treatment, which makes it necessary to have a specically adapted UV coating with very good levelling. We have coatings which are adapted to that application in our range.

    Dieter Zang (FUJIFILM)


    Best regards

  5. #5
    apolloUVGOD is offline Junior Member
    Join Date
    Feb 2011
    Posts
    19

    Default Wave Goodby

    Your Wave e ness,
    A wave or "rivering effect" is this
    1) To much coating , Tighten metering roller 50% of time
    2) Viscosity of coating to high , In winter coating body up and don't flow out as designed so a lower viscosity helps
    3) Keep the coating at 80 degrees , and your boss will think you are an expert.

    Have a smooth future,

  6. #6
    GRAPHIC COATINGS's Avatar
    GRAPHIC COATINGS is offline Junior Member
    Join Date
    Apr 2009
    Posts
    11

    Default

    IR is your friend !

  7. #7
    MalcolmBliss's Avatar
    MalcolmBliss is offline Junior Member
    Join Date
    Sep 2010
    Posts
    17

    Default

    You may try speeding up your machine a little too, that sometimes helps lessen application a little. Or try another brand of coating. Our TEC machine really works better with their brand of coating. Myself, i see little difference in coatings of different brands. However, every shop always has an expert on what they think the job should look like if you get where I'm coming from.....